ASTM A312 TP316
Chemical Requirements: Composition, %, max
Grade | TP316(S31600) |
Carbon | 0.08 |
Manganese | 2.00 |
Phosphorus | 0.045 |
Sulfur | 0.030 |
Silicon | 1.00 |
Chromium | 16.0-18.0 |
Nickel | 11.0-14.0 a |
Molybdenum | 2.00-3.00 |
a For welded TP316 pipe, the nickel range shall be 10.0–14.0 %.
Heat Treating Temperature: 1900 °F [1040 °C]
Tensile Requirements:
Tensile Strength, min ksi [MPa] | 75 [515] |
Yield Strength, min ksi [MPa] | 30 [205] |
Elongation in 2 in. or 50 mm (or 4D), min, %:
Longitudinal | 35 |
Transverse | 25 |