API 5L PSL 2

API 5L – Line Pipe

Chemical composition for PSL 2 pipe with t ≤ 25.0 mm (0.984 in)  max,  %

GradeHeat and product analysesCarbon equivalent a
C bSiMn bPSVNbTiOther
Seamless and welded pipesCEIIWCEPcm
L245R or BR0.240.401.200.0250.015cc0.04e0.430.25
L290R or X42R0.240.401.200.0250.0150.060.050.04e0.430.25
L245N or BN0.240.401.200.0250.015cc0.04e0.430.25
L290N or X42N0.240.401.200.0250.0150.060.050.04e0.430.25
L320N or X46N0.240.401.400.0250.0150.070.050.04d,e0.430.25
L360N or X52N0.240.451.400.0250.0150.100.050.04d,e0.430.25
L390N or X56N0.240.451.400.0250.0150.10f0.050.04d,e0.430.25
L415N or X60N0.24f0.45f1.40f0.0250.0150.10f0.05f0.04fg,has agreed
L245Q or BQ0.180.451.400.0250.0150.050.050.04e0.430.25
L290Q or X42Q0.180.451.400.0250.0150.050.050.04e0.430.25
L320Q or X46Q0.180.451.400.0250.0150.050.050.04e0.430.25
L360Q or X52Q0.180.451.500.0250.0150.050.050.04e0.430.25
L390Q or X56Q0.180.451.500.0250.0150.070.050.04d,e0.430.25
L415Q or X60Q0.18 f0.451.700.0250.015gggh0.430.25
L450Q or X65Q0.18 f0.451.700.0250.015gggh0.430.25
L485Q or X70Q0.18 f0.451.800.0250.015gggh0.430.25
L555Q or X80Q0.18 f0.451.900.0250.015gggi,jas agreed
Welded pipe
L245M or BM0.220.451.20.0250.0150.050.050.04e0.430.25
L290M or X42M0.220.451.30.0250.0150.050.050.04e0.430.25
L320M or X46M0.220.451.30.0250.0150.050.050.04e0.430.25
L360M or X52M0.220.451.40.0250.015ddde0.430.25
L390M or X56M0.220.451.40.0250.015ddde0.430.25
L415M or X60M0.12f0.45f1.60f0.0250.015gggh0.430.25
L450M or X65M0.12f0.45f1.60f0.0250.015gggh0.430.25
L485M or X70M0.12f0.45f1.70f0.0250.015gggh0.430.25
L555M or X80M0.12f0.45f1.85f0.0250.015gggi0.43f0.25
L625M or X90M0.100.55f2.10f0.0200.010gggi0.25
L690M or X100M0.100.55f2.10f0.0200.010gggi,j0.25
L830M or X120M0.100.55f2.10f0.0200.010gggi,j0.25

a Based upon product analysis. For seamless pipe with t > 20.0 mm (0.787 in), the carbon equivalent limits shall be as agreed. The CEIIW limits apply if the carbon mass fraction is greater than 0.12 % and the CEPcm limits apply if the carbon mass fraction is less than or equal to 0.12 %.

b For each reduction of 0,01 % below the specified maximum for carbon, an increase of 0,05 % above the specified maximum for manganese is permissible, up to a maximum of 1,65 % for grades W L245 or B, but u L360 or X52; up to a maximum of 1,75 % for grades > L360 or X52, but < L485 or X70; up to a maximum of 2,00 % for grades W L485 or X70, but u L555 or X80; and up to a maximum of 2,20 % for grades > L555 or X80.

c Unless otherwise agreed, the sum of the niobium and vanadium concentrations shall be u 0,06 %.

d The sum of the niobium, vanadium and titanium concentrations shall be ≤ 0.15 %.

e Unless otherwise agreed, 0.50 % maximum for copper, 0.30 % maximum for nickel, 0.30 % maximum for chromium and 0.15 % maximum for molybdenum.

f Unless otherwise agreed.

g Unless otherwise agreed, the sum of the niobium, vanadium and titanium concentrations shall be ≤ 0.15 %.

h Unless otherwise agreed, 0.50 % maximum for copper, 0.50 % maximum for nickel, 0.50 % maximum for chromium and 0.50 %

i Unless otherwise agreed, 0.50 % maximum for copper, 1.00 % maximum for nickel, 0.50 % maximum for chromium and 0.50 % maximum for molybdenum.

j 0.004 % maximum for boron.

 

Requirements for the results of tensile tests for PSL 2 pipe 

Pipe gradePipe body of seamless and welded pipesWeld seam of HFW, SAW and COW pipes
Yield strength 

Rt0,5 b Mpa

Tensile strength a

Rm Mpa

Ratio a, b, c

Rt0,5/Rm

Elongation

A%

Tensile strength d

Rm Mpa

L245R or BR245450 e4157600.93 f415
L245N or BN
L245Q or BQ
L245M or BM
L290R or X42R2904954157600.93 f415
L290N or X42N
L290Q or X42Q
L290M or X42M
L320N or X46N32052542357600.93 f435
 L320Q or X46Q
L320M or X46M
L360N or X52N3605304607600.93 f460
L360Q or X52Q
L360M or X52M
L390N or X56N3905454907600.93 f490
L390Q or X56Q
L390M or X56M
L415N or X60N4155655207600.93 f520
L415Q or X60Q
L415M or X60M
L450Q or X65Q4506005357600.93 f535
L450M or X65M
L485M or X70M4856355707600.93 f570
 L485Q or X70Q
L555Q or X80Q5557056258250.93 f625
L555M or X80M
L625M or X90M6257756959150.95 f695
L690M or X100M6908407609900.97 f760
L830M or X120M830105091511450.99 f915

a For intermediate grades, the difference between the specified maximum yield strength and the specified minimum yield strength shall be as given in the table for the next higher grade, and the difference between the specified minimum tensile strength and the specified minimum yield strength shall be as given in the table for the next higher grade. For intermediate grades lower than Grade L555 or X80, the tensile strength shall be u 760 MPa (110 200 psi). For intermediate grades higher than Grade L555 or X80, the maximum permissible tensile strength shall be obtained by interpolation. For SI units, the calculated value shall be rounded to the nearest 5 MPa. For USC units, the calculated value shall be rounded to the nearest 100 psi.

b For grades > L625 or X90, Rp0,2 applies.

c This limit applies for pipe with D > 323,9 mm (12.750 in).

d For intermediate grades, the specified minimum tensile strength for the weld seam shall be the same value as was determined for the pipe body using footnote a).

e For pipe with D < 219,1 mm (8.625 in), the maximum yield strength shall be u 495 MPa (71 800 psi).

f The specified minimum elongation, Af, shall be as determined using the following equation:

A = C AXC0.2/U0.9

where

C is 1 940 for calculations using SI units and 625 000 for calculations using USC units;

Axc is the applicable tensile test piece cross-sectional area, expressed in square millimeters (square inches), as follows:

— for circular cross-section test pieces, 130 mm2 (0.20 in2) for 12,5 mm (0.500 in) and 8,9 mm (0.350 in) diameter test pieces; and 65 mm2 (0.10 in2) for 6,4 mm (0.250 in) diameter test pieces;

— for full-section test pieces, the lesser of a) 485 mm2 (0.75 in2) and b) the cross-sectional area of the test piece, derived using the specified outside diameter and the specified wall thickness of the pipe, rounded to the nearest 10 mm2(0.01 in2);

— for strip test pieces, the lesser of a) 485 mm2 (0.75 in2) and b) the cross-sectional area of the test piece, derived using the specified width of the test piece and the specified wall thickness of the pipe, rounded to the nearest 10 mm2 (0.01 in2);

U is the specified minimum tensile strength, expressed in megapascals (pounds per square inch).

g. Lower Rt0,5/Rm ratio values may be specified by agreement for L690 or X100 and L830 or X120 pipe.